Cast iron is difficult, but not impossible, to weld. In most cases, welding on cast iron involves repairs to castings, not joining casting to other members. The repairs may be made in the foundry where the castings are produced, or may be made to repair casting defects that are discovered after the part is machined. Mis-machined cast iron parts may require repair welding, such as when holes are drilled in the wrong location. Frequently, broken cast iron parts are repaired by welding. Broken cast iron parts are not unusual, given the brittle nature of most cast iron.
While there are a variety of types of cast iron, the most common is gray cast iron, and these guidelines are directed toward this type of material.

A few facts about cast iron help in understanding the welding challenges. Cast iron typically has a carbon content of 2% - 4%, roughly 10 times as much as most steels. The high carbon content causes the carbon to form flakes of graphite. This graphite gives gray cast iron its characteristic appearance when fractured.

When castings are made, molten iron is poured into a mold and allowed to slowly cool. When this high carbon material is allowed to cool slowly, crack free castings can be made. Remembering this is helpful when welding cast iron: during and after welding, the casting must either be allowed to cool slowly, or should be kept cool enough that the rate of cooling is not important.

A critical temperature in most cast iron is about 1450 degrees F. When at this temperature, conditions that can lead to cracking occur. While the arc will heat the casting to temperatures above this level, it is important that the casting not be held at this temperature for long periods of time.

Electrode Selection
If the part is to be machined after welding, a nickel-type electrode will be required. Use Lincoln Softweld® 99Ni stick electrode for single pass, high dilution welds. Softweld 55 Ni is preferred for multiple pass welds. Sometimes, root passes are put in with Softweld 99 Ni, followed by fill passes with Softweld 55 Ni. For welds where machining is not required, and where the weld is expected to rust like the cast iron, Lincoln Ferroweld® stick electrode can be used.

To Heat, or not to Heat
In general, it is preferred to weld cast iron with preheat--and lots of it. But, another way to successfully weld cast iron is to keep it cool--not cold, but cool. Below, both methods will be described. However, once you select a method, stick with it. Keep it hot, or keep it cool, but don't change horses in the middle of the stream.

Welding Techniques with Preheat
Preheating the cast iron part before welding will slow the cooling rate of the weld, and the region surround the weld. It is always preferred to heat the entire casting, if possible. Typical preheat temperatures are 500-1200 degrees F. Don’t heat over 1400 degrees F since that will put the material into the critical temperature range. Preheat the part slowly and uniformly.

Weld using a low current, to minimize admixture, and residual stresses. In some cases, it may be necessary to restrict the welds to small, approximately 1-inch long segments to prevent the build up of residual stresses that can lead to cracking. Peening of weld beads can be helpful in this regard as well.

After welding, allow the part to slowly cool. Wrapping the casting in an insulating blanket, or burying it in dry sand, will help slow cooling rates, and reduce cracking tendencies.

Welding Techniques without Preheat
The size of the casting, or other circumstances, may require that the repair be made without preheat. When this is the case, the part needs to be kept cool, but not cold.

Raising the casting temperature to 100 degrees F is helpful. If the part is on an engine, it may be possible to run it for a few minutes to obtain this temperature. Never heat the casting so hot that you cannot place your bare hand on it.

Make short, approximately 1” long welds. Peening after welding is important with this technique. Allow the weld and the casting to cool. Do not accelerate the rate of cooling with water or compressed air. It may be possible to weld in another area of the casting while the previous weld cools. All craters should be filled. Whenever possible, the beads should be deposited in the same direction, and it is preferred that the ends of parallel beads not line up with each other.

Sealing Cracks
Because of the nature of cast iron, tiny cracks tend to appear next to the weld even when good procedures are followed. If the casting must be water tight, this can be a problem. However, leaking can usually be eliminated with some sort of sealing compound or they may rust shut very soon after being returned to service.

The Studding Method

One method used to repair major breaks in large castings is to drill and tap holes over the surfaces that have been beveled to receive the repair weld metal. Screw steel studs into the threaded holes, leaving 3/16” (5 mm) to ?” (6 mm)of the stud above the surface. Using the methods discussed above, weld the studs in place and cover the entire surface of the break with weld deposit. Once a good weld deposit is made, the two sides of the crack can be welded together.


ABOUT  KEVA
Keva Casting is a professional casting company that focuses on Construction, Machinery, Automobile, Hardware, Pipeline and many other industries.
We provide top quality products with the best service based on our complete production chain including our own mold design, advanced production techniques, and full management of the supply chain. Keva Casting has two factories located in Zhucheng, China's Shandong province.
We use "shell molding", which is a new technique that has been developed in recent years.This new technique has simplified production procedures and reduced air pollution compared with traditional sand casting and investment casting. Shell making and core making are faster to ensure production in enormous quantities. The dimensions and surface finishing are satisfactory for all kinds of industrial requirements. Besides supplying our own formwork & scaffolding systems, our casting products also supply OEM services in various industries.

AV无码久久久久不卡网站下载| 交换交换乱杂烩系列yy| 男男双龙调教失禁高潮play| 女人下边被添全过程A片| 欧美FREESEX潮喷| 精品国产天线2024| 亚洲高清免费观看在线视频| 精品无码久久久久久久久久| 精品久久久久久中文字幕无码VR| 加勒比色综合久久久久久久久| 自拍偷在线精品自拍偷99| 无码人妻精品一区二区三18禁| 无码国产69精品久久久久网站| 97无码免费人妻超级碰碰碰碰| 欧美日韩无套内射另类| 全部免费的毛片在线看| 国产成人亚洲影院在线播放| 看曰本女人大战黑人视频| 一二三四视频在线观看日本| 亚洲中文字幕无码久久精品1| A级毛片无码久久精品免费| 国产精品亚洲一区二区三区在线| 亚洲成A人片在线观看无码3D| 国产97视频人人做人人爱| 人妻少妇无码精品视频区| 国产后入清纯学生妹| 亚洲一本大道无码av天堂| 99在线精品国自产拍不卡| 暴力调教一区二区三区| 欧洲亚洲精品A片久久99动漫| 美女免费高清观看影视大全| 在线观看片免费视频无码| 色偷偷噜噜噜亚洲男人| 曰批视频免费看30分钟| 97亚洲狠狠色综合蜜桃| 在线观看片免费人成视频无码| 最新国产在线拍揄自揄视频| 国产综合视频一区二区三区| 亚欧乱色熟女一区二区三区| 亚洲精品久久久久久久久AV无码| 中字幕久久久人妻熟女天美传媒|