Defects Caused by Improper Cooling after Forging

2024-07-05
Defects caused by improper cooling after forging


Cooling cracks:


The cracks are smooth and slender, sometimes in the form of mesh cracks. High magnification observation: martensitic structure appears near the crack, and there is no trace of plastic deformation. It mostly occurs on martensitic steel forgings. Due to the rapid cooling after forging, large thermal stress and structural stress are generated. Slow cooling in a sandpit or slag around 200°C can prevent such cracks.

Cooling deformation:

Large, thin-walled, thin-ribbed frame members, warping deformation during post-forging cooling. It is caused by the interaction of residual stress generated in forging and stress caused by uneven cooling. Annealing immediately after forging can prevent such defects.

475℃ brittle crack:

Surface cracks appear when ferritic stainless steel is cooled too slowly after forging, and the residence time is too long in the temperature range of 400-520 °C. Due to the long residence time at 400-520 °C, a special substance is precipitated and brittleness is caused. Fast cooling at 400-520°C can prevent cracks.

Mesh Carbide:

Carbides are precipitated in the form of a network along the grain boundaries, which reduces the plasticity and toughness of the forgings. This defect is often seen in steel forgings with high carbon content. Due to the slow cooling after setting, the carbides can be folded along the grain boundaries, which makes the forgings easy to crack during quenching and deteriorates the performance of the parts.



ABOUT  KEVA
Keva Casting is a professional casting company that focuses on Construction, Machinery, Automobile, Hardware, Pipeline and many other industries.
We provide top quality products with the best service based on our complete production chain including our own mold design, advanced production techniques, and full management of the supply chain. Keva Casting has two factories located in Zhucheng, China's Shandong province.
We use "shell molding", which is a new technique that has been developed in recent years.This new technique has simplified production procedures and reduced air pollution compared with traditional sand casting and investment casting. Shell making and core making are faster to ensure production in enormous quantities. The dimensions and surface finishing are satisfactory for all kinds of industrial requirements. Besides supplying our own formwork & scaffolding systems, our casting products also supply OEM services in various industries.


高清国产精品人妻一区二区| mm1313亚洲国产精品久久| 国产成人亚洲精品青草天美| 色综合久久久无码中文字幕波多| 黑人粗大猛烈进出高潮视频| 欧美性猛交XXXX乱大交3| 国产va免费精品观看精品| 无码少妇一区二区三区视频| 免费古装a级毛片无码| 女人扒下裤让男人桶到爽| WWW.久久.COM| 亚洲AV无码久久| 精品产区WNW2544| 丰满人妻一区二区三区视频53| 欧美成人看片黄a免费看| 国产精品乱码高清在线观看| 蜜臀av国内精品久久久较| 三年片免费大全国语| 亚洲女毛多水多21p| 欧美成人精品高清在线观看| 领导在办公室含我奶头小短文| 欧美性开放情侣网站| 一区二区三区四区在线不卡高清| 亚洲综合成人婷婷五月在线观看| 国产精品久久国产精品99| 精品一区精品二区| 精品爆乳一区二区三区无码AV| 日韩免费高清大片在线| 永久免费AV无码入口国语片| 小蜜被两老头吸奶头在线观看| 伊人直播网站| 久久久久夜夜夜精品国产| 男ji大巴进入女人的直播| 妇女性内射冈站HDWWW000| 97亚洲精华液| 午夜成人亚洲理论片在线观看| 久久婷婷香蕉热狠狠综合| 黄床大片免费30分钟国产精品| 亚洲乱码av中文一区二区| 狠狠色丁香久久婷婷综合_中| 亚洲精品久久无码AV片银杏|